Learning how to tan a hide means learning a chain of steps, and the tan you brush on or soak the skin in is only one link. You flesh it, salt it, rehydrate it, pickle it, thin it, neutralize it, tan it and oil it, then either dry and break it into soft leather or freeze it wet for a mount. Skip a link and the hide tells you later, usually as bald patches or a skin that dries stiff. Below: the whole process for hair-on hides, the method families, supply costs, and when a tannery makes more sense.
What does tanning do that salting and drying don't?
Tanning changes the skin itself. The EPA's chapter on the leather industry describes tanning as "the reaction of collagen fibers in the hide with tannins, chromium, alum, or other chemical agents" (EPA AP-42, section 9.15). Salt doesn't do that. A salted, dried skin is still a raw skin, and soaking it in water brings it back.
Van Dyke's pickling instructions put salt's job plainly: "Salting removes skin moisture and sets the hair" (Van Dyke's, Pickling). That's preparation. You can watch the difference in a full tanning demonstration by Amy, a North Carolina taxidermist (Amy's Taxidermy, 2023): a wolverine pelt salted "6 months or so" and "really salt dried hard" goes into a rehydration bath with a relaxer added, then the pickle, the same sequence as the fresh bobcats. For Lutan FN, Liqua Tan and Curatan, Van Dyke's says "you must salt and pickle" before the tan goes on (Van Dyke's, Hide Tanning).
What are the stages of tanning a hide?
Most hair-on tanning runs in the same order: flesh, salt, rehydrate and wash, pickle, shave, degrease if needed, neutralize, tan, oil, then dry and break the hide or bag and freeze it for mounting. Figures below come from Van Dyke's Lutan FN sheet and Amy's McKenzie demonstration; where your product's sheet differs, follow it.
- Flesh. Remove as much meat and fat as you can, split the lips and turn the ears, and pull the cartilage from the nose (Van Dyke's Lutan FN Kit Instructions). Amy also turns the feet "all the way down to the claw" and splits the tails.
- Salt. Rub fine-ground, non-iodized salt into the flesh side and leave it 12 to 24 hours, per the Lutan FN sheet; Van Dyke's pickling page says 24 to 48 hours. Amy salts overnight and then gives the hides a second salting. When salt turns to slush, a HuntingNet member (M.Magis, 2005) says to "shake off the wet salt and apply new" and set the hide on an incline (forum post, 2005).
- Rehydrate and wash. Soak the skin soft, checking often (Amy: "you don't want to leave them in the rehydration bath any longer than you have to"), and rinse out the blood, since "the pickle will tend to set that blood stain in."
- Pickle. The Lutan FN sheet gives, per gallon of water, 1 lb of salt plus one acid (1/2 oz of McKenzie Ultimate Acid, 3 oz of pickling crystals or 1 oz of oxalic acid), with a pH of 1.5 to 2.0 and at least 72 hours in the pickle. Amy aims for 1.5 and adds acid when it rises; she wants it back "below a two." Putting a bobcat into the pickle, Amy says, "If you have sensitive skin or if you're smart, yes, I would probably suggest wearing some gloves" (video, 24:34).
- Shave. Thin the skin while it's pickled. Van Dyke's: "The thinner the skin is shaved the softer and more flexible it will be." Amy's rule for bobcats and deer capes is "3 days in the pickle, then shave, then return for at least 24 hours" (video, 32:09).
- Degrease if needed. Bear, raccoon and beaver "all will require degreasing," per Van Dyke's: McKenzie Relaxer/Degreaser at 2 fluid oz per gallon for 30 minutes, or Dawn at 1/2 fluid ounce per gallon for light jobs.
- Neutralize. A baking soda bath raises the pH so the tan can bond. Van Dyke's uses 1 ounce per gallon, 15 minutes for light-skinned animals and 20 for deer. Amy mixes 1 tablespoon per gallon, soaks bobcats and coyotes 20 minutes and gives thick hides like elk longer, aiming to bring the skin from about pH 2 up "to about a four to five" (video, 33:05).
- Tan. Brush it on or submerge the skin. For Lutan FN, the sheet calls for pH 3.5 to 4, 12 to 24 hours for small game or a well-shaven deer cape, 24 to 48 hours for elk, moose and caribou, and never more than 48 hours. Van Dyke's Hide Tanning page gives shorter times for its own mix (16 to 18 hours on deer and 20 to 22 on elk or moose), so go by the sheet that came with your Lutan FN. For the rub-on Syn-Oil Tan, that page says, "With latex gloves, rub the Syn-Oil, tan thoroughly into the cape" (Van Dyke's, Hide Tanning).
- Oil. Submersion tans need oil afterward. Amy says tans like Lutan F or EZ-100 "require an additional oiling"; the Lutan FN sheet mixes McKenzie Leather Oil with hot water, 1 part oil to 2 parts water.
- Freeze or finish. After the oil has soaked in "a minimum of 8 hours," Van Dyke's says the skin can be mounted or rolled up, bagged and frozen. For rug work or furs, it "should be stretched and broken as it dries."
Wet tan or dry tan: which one do you need?
A wet tan stays damp and goes into the freezer until mounting day; a dry tan is dried and broken soft for rugs and wall hangers. A HuntingNet member posting in 2011 said a customer sees no difference in a mount: same chemicals, same lifespan, but a dry tan "will need to be re-hydrated before mounting."
That member (TimberlandTaxidermy) added that after using both commercially wet and dry tanned hides, they "noticed no difference in stretch" once rehydrated (forum post, 2011). Amy splits her batch the same way: mount skins get bagged and frozen, rug skins get dried and broken, and on a bobcat rug she leaves the head unstretched because "this is going to be rehydrated and mounted" (video, 45:53).
Not everyone has had that luck. An AfricaHunting member (MarkB, 2023) wrote, "We use wet tan for mounts, cannot ship wet tan to NA," and said a batch once dry tanned in Africa came back as "rubber hides" that had to go to the member's own tannery before mounting (forum post, 2023). His advice: ask your taxidermist what they want or prefer.
Which tanning method should you use for a hide?
For hide tanning at home with the hair on, you're choosing between an alum-and-salt kit, a brush-on tan over an acid pickle, and a submersion tan over an acid pickle. Chrome is what the commercial leather industry mostly runs. Brain tanning is mostly used for hair-off buckskin, which has its own guide; the Missouri Department of Conservation notes the bucking step "is only used in hair-off tanning."
| Method family | Examples | How it goes on | What the source says |
|---|---|---|---|
| Alum and salt | Potassium Alum Tanning Kit, ammonium alum, aluminum sulfate | Kit or bulk chemical | EPA lists alum among tanning agents; Van Dyke's sells the kit and bulk alum (Van Dyke's) |
| Brush-on tan over a pickle | McKenzie Tan, Liqua Tan, Syn-Oil Tan, Curatan | Brushed or rubbed into the flesh side | Syn-Oil absorbs "a minimum of 6 hours," then mount, freeze or stake and break; Curatan wants a room of 70 to 80 degrees Fahrenheit (Van Dyke's, Hide Tanning) |
| Submersion tan over a pickle | Lutan FN, EZ-100, Tannium | Skin soaked in a tan bath | Lutan FN "will only tan properly between 3.5 and 4"; needs oiling afterward (Van Dyke's; Amy's Taxidermy) |
| Chrome | Basic chromium sulfate | Commercial one-bath process | About 90 percent of US tanning production; hides start pickled at pH 3 or lower (EPA) |
| Brain (buckskin) | Buckskin | Usually hair removed first | Bucking, a soak in a high-pH hydrated lime solution, "is only used in hair-off tanning" (Missouri Department of Conservation) |
Brush-on tans are simple to apply. Amy's pitch for McKenzie Tan: "Can you paint a house? ... You can operate a paintbrush" (video, 36:09). She makes sure the eyelids get covered, "a common place to get shrinkage." Submersion tans take more babysitting: Lutan FN below pH 3.5 "will surface tan the skin, and above will precipitate the chemical" (Van Dyke's), so you test and adjust during the soak. Van Dyke's also lists Krowtann 2000 and a Krowtann Whitetail Formula; follow the instructions that ship with the bottle.
What tools do you need to tan hides at home?
Less than you might think: a fleshing knife and beam, fine salt, plastic tubs or 5-gallon buckets, an acid, baking soda, low-range pH strips, a scale and measuring spoons, a brush and something to break the hide on. Amy calls her fleshing machine and sawdust tumbler useful but not absolute must-haves.
Some of the product links below are affiliate links. Taxidermy Hobbyist may earn a commission on qualifying purchases at no extra cost to you. See our affiliate disclosure.
- Fleshing knife and beam. A Rokslide member (EdP, 2024) wrote that you "can get away with a cheap dull knife" on fox, possum and muskrat, but "will want a sharp knife for beaver, otter, coyote, deer, bear, raccoon," and that the beam should match the knife's curve (forum post, 2024). Browse a fleshing knife, or see our guide to taxidermy knives and fleshing tools.
- Shaving. For a few pelts, Amy says you can shave with "a knife or a scalpel" instead of a machine (video, 29:52).
- Tubs. Amy tans in 100- and 75-gallon tubs but says "you can tan in a five gallon bucket" for smaller batches, using at least 3 or 4 gallons per deer cape and 2 to 3 per bobcat. Van Dyke's wants at least 5 gallons of pickle for a full shoulder deer cape.
- pH strips. Amy buys strips that "only go up to a three" from a taxidermy supplier, because pool strips focus on higher pH (video, 8:08).
- Breaking tools. A board or table edge, a scraper and a palm sander (Amy). Van Dyke's says a household dryer can tumble a hide only on a "NO heat" setting.
- A kit, if you'd rather start simple. Browse a hide tanning kit or buy one of the supplier kits priced below.
What do hide tanning supplies cost?
The chemicals are the cheap part. Van Dyke's listed its McKenzie Tan Tanning Kit at $26.50 and a 1 lb Lutan FN kit at $41.00 on November 22, 2026 (Van Dyke's, Tanning Kits). The kits bundle what you need for a first hide; the chemicals are also sold on their own by the quart or pound.
| Item | Size | Van Dyke's price, Nov 22, 2026 |
|---|---|---|
| McKenzie Tan Tanning Kit | Kit | $26.50 (kits) |
| Potassium Alum Tanning Kit | Kit | $29.00 (kits) |
| Curatan Kit | Hair on | $35.00 (kits) |
| Lutan FN Kit | 1 lb | $41.00 (kits) |
| McKenzie Tanning Kit with DVD | Kit | $41.50 (kits) |
| Lutan FN Kit | 4 lb | $80.50 (kits) |
| Liqua Tan | Quart | $31.00 (chemicals) |
| Krowtann 2000 | Quart | $33.50 (chemicals) |
| Lutan FN | 5 lb | $42.00 (chemicals) |
| Ammonium Alum | 5 lb | $23.50 (chemicals) |
"Salt is cheap," as Amy puts it: she buys 50 lb bags of fine stock salt and said in 2023, "These are about $7" (video, 7:43). For how the McKenzie line compares as a supplier, see our McKenzie Taxidermy Supply review.
Should you tan a hide yourself or send it to a tannery?
Tan it yourself for practice, a wall hanger or a rug you'll forgive; send out a cape you can't replace. An Idaho trapper on HuntTalk (brymoore, 2025) who had tanned furs, deer and elk at home wrote, "it's a lot of work. My hides were never quite right," and now sends hides to a tannery.
The member calls the tannery's cost "relatively cheap" (forum post, 2025). Our list of commercial tanneries shows the ones in our directory, by state. Home results can work, though. A Rokslide member (Haggin, 2021) whose daughter tanned her whitetail doe for a 4-H project advised: "Spend time fleshing, then spend some more." She had "no hair slippage" and softened the flesh side with an orbital sander (forum post, 2021).
Tannery prices vary with the animal and how much prep you've done. These are single reports from forum members, not a market range:
- A HuntTalk member (noharleyyet) reported in 2025 that a cow elk hide their son had done at a tannery in Denton cost, as the member recalled, "circa $320" (forum post, 2025).
- A HuntingNet member (ArcticBowMan) wrote in 2004 that for tanning just a bear hide you could expect "about $40-$50 a foot, depending on how much work is left for the tannery" (forum thread, 2004).
- A Rokslide member (Pochuck) posted a 2025 quote of $1,200 per musk ox cape for tanning, and said a local taxidermist told the member capes "should be around $450" (forum thread, 2025).
- An AfricaHunting member (CloudySkies) called a 2026 quote of about $510 for a wildebeest flat skin and $350 for a nyala "bordering on outrageous" (forum post, 2026).
Turnaround is the other cost. A HuntingNet member (wingchaser_labs, 2009) wrote that "most tanneries take 3 months during the peak of the season maybe 4 at most" (forum post, 2009). Another (Western MA Hunter, 2009) said the local shop the member believed tans in-house had a 6-month wait, against a year and two years at two shops that ship hides to a commercial tannery (forum post, 2009). The same member said hides they sent out themselves usually came back in about 3 to 4 weeks. When you find a taxidermist for a mount, ask who does the tanning and where.
Why do home-tanned hides fail?
Most of these failures trace back to a step the instructions already warn about: hair slip, stiff leather and greasy skins usually come from a skin left raw too long, a guessed pH, or a bad neutralizing, salting or degreasing step.
- Hair slip. Van Dyke's warns that "the longer the hide remains in its raw state, the more likely the hair is to slip," and says a low-pH pickle "in most cases assures the killing of bacteria that causes hair slippage." Amy: "if you're guessing on your pH then your hides are very likely going to slip" (video, 9:11). An AfricaHunting member (harden, 2019) reads slip by location on a safari kudu: around the eyes, nose and lips it is "the PH's fault," meaning the professional hunter's; on the shoulders or neck the member blames the tannery or a taxidermist doing his own tanning, citing "bad tan, high ph levels and not thinning hides for pickle to penetrate" (forum post, 2019).
- Hard, stiff leather. If the pH is too low before tanning, Van Dyke's says most tans "will rapidly fix to the skins surface with little or no penetration," and the interior "will become stiff on drying." Skipping the neutralizing bath risks exactly that. Dry skins also need working: in its Curatan steps, Van Dyke's says to work them "several minutes each day while drying."
- Over-neutralizing. Too long in the soda bath gives "slow and unfixing penetration of tannins," so Van Dyke's says "it is still always best to neutralize for a short interval."
- Skipping the salt. Amy says salting isn't "an absolute necessity in most cases," but without it the blood and moisture come out in the pickle and push the pH up, so she uses more acid. Her rule: "salt it overnight for at least 12 hours" (video, 51:27).
- Wrong salt. Van Dyke's: "Never use rock salt or reuse old salt!" Amy wants salt that looks like table salt and says iodized or not doesn't matter to her; rock salt clouds the pickle and doesn't dissolve as well (video, 6:25).
- Bad pH testing. After a day, Amy's pickle had drifted "up into that two to two and a half range," which she calls too high, so she added acid (video, 28:22).
- Grease left in. On bear, raccoon or beaver, skipping the degreaser leaves "an oily finished hide," which Amy says can affect the mount later (video, 25:35).
Which tanning guide fits your animal?
How to tan an animal hide changes a little by species, though the steps above apply to most hair-on mammal skins. Deer, brain-tanned buckskin, furbearer pelts and rabbit skins each have their own guide on this site, so pick the page that matches the skin on your bench.
- Deer. Hair-on capes and hides or buckskin: our guide to tanning a deer hide with the hair on or off.
- Hair-off buckskin the old way. The brain tanning method has its own guide.
- Furbearers. Pelts for wall hangers and rugs: tanning fur pelts at home.
- Rabbits. Rabbit skins get their own page: tanning rabbit skins.
For skinning and mounting around the tanning step, the step-by-step mammal mounting process picks up where this page stops.
Frequently asked questions
How long does it take to tan a hide?
Plan on the better part of a week, most of it waiting. On the Lutan FN sheet, salting takes 12 to 24 hours, the pickle at least 72 hours, the tan 12 to 24 hours for small game or a well-shaven deer cape, and the oil at least 8 hours before mounting or freezing. Tanning hides for a dry finish adds drying and breaking on top of that.
Do you have to pickle a hide before tanning?
For Lutan FN, Liqua Tan and Curatan, Van Dyke's says "you must salt and pickle" first. The pickle also buys time: Van Dyke's calls it "a safe place to store a hide as long as the pH is below 2.0" if you can't get to it right away.
What pH should a tanning pickle be?
Van Dyke's Lutan FN sheet gives 1.5 to 2.0 for the pickle and 3.5 to 4 for the Lutan FN tan bath. Amy aims for 1.5 in the pickle and neutralizes the skin to about 4 to 5 before her brush-on tan. Use low-range strips so you can read the difference.
Sources
- Amy's Taxidermy, "Step-By-Step COMPLETE TANNING TUTORIAL! Taxidermy WET and DRY tans!" (YouTube, 2023)
- Van Dyke's, Lutan FN Kit Instructions
- Van Dyke's, Hide Tanning
- Van Dyke's, Pickling
- Van Dyke's, Tanning Kits (prices read November 22, 2026)
- Van Dyke's, Tanning Chemicals (prices read November 22, 2026)
- US EPA, AP-42 Section 9.15, Leather Tanning
- Missouri Department of Conservation, "Making Buckskin"
- HuntingNet, "wet tan or dry?" (2011)
- HuntingNet, "Salt Curing How To" (2005)
- HuntingNet, "Price on bear tanning?" (2004)
- HuntingNet, "Average wait for a deer mount," post 2 (2009)
- HuntingNet, "Average wait for a deer mount," post 4 (2009)
- AfricaHunting, "Tanning vs Dip/Pack" (2023)
- AfricaHunting, "Hair slippage or normal characteristic" (2019)
- AfricaHunting, "Flat Skin Tanning Cost" (2026)
- HuntTalk, "Tanning you own furs?" (2025)
- HuntTalk, "Tanning you own furs?," post 6 (2025)
- Rokslide, "DIY tanning" (2021)
- Rokslide, "Fleshing tool recommendation" (2024)
- Rokslide, "Musk Ox Tanning Price" (2025)